Welcome to GreenMore
Thin-film three-curve solar tiles are one of the most architecturally integrated BIPV options on the market. Their curved CIGS (copper indium gallium selenide) layer, ETFE front film and laminated edge sealing let them replace conventional roof tiles while generating electricity. That multi-layer build is exactly what makes them attractive — and what introduces a specific failure mode that project teams should understand: ETFE surface delamination, commonly described on site as "peeling" or "lifting."
In almost every case it starts at the edge rather than at the cell, and it takes a season or two before anyone notices. By the time it is visible on the roof, the area that has actually failed is usually larger than the area you can see.
The front film has peeled back to a pale patch on one tile, and the edge seal beside it has cracked.
A curved solar tile is not a flat panel bent into shape. It is a laminated composite built from the outside in:
The curved profile adds a permanent bending stress that flat panels do not carry. ETFE is chemically inert by nature, which is a good thing for durability, but it also means the surface must be specially treated (corona, plasma or primer) before the encapsulant will bond to it reliably. If that surface treatment is inconsistent, the interface between ETFE and encapsulant becomes the weakest link in the stack.
Think of it as a multi-layer sticker on a curved surface. If the adhesive at the edge starts to lift, moisture and air get under the layers, and the lifting spreads. In a solar tile, that "lifting" is delamination.
Curved tiles are not built on one cell technology alone. CIGS is the thin-film route; back-contact crystalline is the other, and the two behave differently once they are on a roof. A comparison of the two routes covers where each one makes sense.
Delamination has a recognizable appearance that differs from common surface defects. The main visual signs are:
These signs are distinct from other common issues:
| Issue | How it differs from delamination |
|---|---|
| Surface dirt or bird droppings | Washes off; does not affect film adhesion |
| Scratches or abrasion | Linear marks on the ETFE surface, no separation |
| Hail damage | Localized puncture or crack, usually with a clear impact point |
| Hot-spot yellowing | Discoloration of the cell layer, no film lifting |
Visual inspection is the first step. Where delamination is suspected, two lab tests give a clearer picture:
Four defects that get mistaken for each other. Only the fourth is delamination.
Delamination is rarely a single-cause event. It is a chain of conditions that, once started, tends to accelerate.
The side seal is the first barrier against moisture. If it degrades, cracks, or is mechanically damaged during installation, rain and humidity can enter the tile interior along the edge. Edge ingress is the dominant moisture path in fielded modules, and the mechanism is well documented by the US Department of Energy.
Once water reaches the ETFE–encapsulant interface, it begins to hydrolyze the adhesive bond. Encapsulants are designed to be moisture-resistant, not moisture-proof at a compromised edge. The bond weakens progressively rather than failing all at once. Studies of EVA adhesion under combined UV, heat and humidity show the same pattern: the loss is cumulative, not sudden (OSTI).
Once the seal is breached, three categories of factor determine how quickly and how far delamination spreads.
A single impact event — hail, a falling branch, dropped tools during maintenance — can create a small breach in the ETFE or edge seal. If the breach is not detected and sealed, it becomes a new entry point for moisture, and the delamination process begins from that point.
Where moisture gets in. A failed edge seal opens a path along the ETFE–encapsulant interface.
The consequences are not cosmetic. Once the ETFE separates from the layers beneath, the tile stops working as a panel and as a roof at the same time.
The delaminated zone no longer transmits light cleanly to the CIGS cell. Output from that area drops. If moisture reaches the cell layer itself, it can corrode the thin-film electrodes, causing a progressive and irreversible power loss that extends beyond the visibly affected area.
Moisture inside the tile reduces insulation resistance. In a string of tiles at system voltage, reduced insulation can lead to leakage current to ground or, in the worst case, DC arcing at a damaged interconnect. Both conditions are safety issues, not just performance issues.
The tile is simultaneously a power generator and a roof covering. A failing edge seal means the tile is also failing as a waterproofing element. Water that enters through a delaminated edge can migrate into the roof structure, with consequences for insulation, battens and the building interior.
A delaminated tile cannot be reliably repaired on the roof. The multi-layer bond cannot be restored in situ. The correct response is replacement of the affected tile(s) and investigation of why the failure started, so the same issue does not recur across the installation.
Edge sealing decides how long the tile lasts, and it is still done by hand, on the roof.
When delamination is reported or suspected on a project, the following steps help separate a single-event damage case from a systemic issue.
| Step | What to do | What it tells you |
|---|---|---|
| 1 | Map the extent | One tile points to impact. A cluster on one roof plane points to drainage or substrate flatness. Spread across orientations points to the product or the sealant. |
| 2 | Check overlaps and fixings | Ponding water, distorted tiles or over-tightened clamps in the affected area. |
| 3 | Record batch and installation dates | Lets you cross-reference other projects built from the same production run. |
| 4 | Send samples for lab testing | EL imaging, insulation resistance and damp-heat aging separate adhesion failure from moisture corrosion. |
| 5 | Set the replacement scope | Affected tiles plus same-batch tiles showing early signs, with the root cause fixed before anything goes back on. |
A BIPV tile is a building component, and that is the harder job of the two. A roof that leaks has failed, whatever the meter says. That means the materials, the manufacturing process, the roof design, and the installation all have to be right. Most cases have more than one cause, and the fix is never a single step.
GreenMore builds curved CIGS thin-film tiles and BC three-curve tiles at its own plant, and supplies BIPV projects in Europe and the Middle East. Our role as the tile manufacturer is to stay in the project from the early feasibility stage — reviewing roof design, confirming product suitability, and providing technical guidance through installation and commissioning — rather than shipping a pallet and walking away. For partners planning a curved solar tile roof, we can review the roof layout, confirm the tile model and configuration, and provide a project-specific proposal. Reach us through our contact page or at export@gmsolarkit.com.
For how that looks on a finished roof, see the Israel home solar roof project. Non-standard profiles, colours and fixing details are handled under customised services.
Partially, yes. The undamaged areas of the tile will continue to produce power. But the delaminated zone no longer contributes, and moisture ingress can progressively corrode the cell layer. A delaminated tile should be replaced rather than left in service, both for performance and for electrical safety.
No. The multi-layer bond cannot be restored in situ. Attempting to re-seal or re-laminate a delaminated tile on the roof does not restore the original adhesion or insulation properties. The correct action is tile replacement.
High-humidity coastal regions, areas with large day–night temperature swings (desert climates), and regions with freeze–thaw cycles all accelerate the conditions that lead to delamination. Projects in these climates should place extra emphasis on edge-seal material selection, overlap drainage design, and post-installation inspection.
Latent defects from lamination or ETFE surface treatment usually surface within the first two to three years, often after the first hot season followed by the first wet one. Damage caused during installation or by a single impact can appear within months. If a tile is going to peel, the first two years are when it shows.
Updated November 11, 2026
Standards referenced: IEC 61215 (module design qualification), IEC 61730 (module safety qualification), EN 14782 (self-supporting metal sheet for roofing).
Stay up to date with GreenMore. We share new BIPV solar tile releases, product and certification updates, and field notes from our projects — no fluff, just the things that matter to installers, distributors, and system integrators. If there's something you'd like to see covered, drop us a line — we read every reply.
Copyright @ 2026 GreenMore All Rights Reserved.